當前位置:首頁產(chǎn)品中心OssilaOssila材料PTB7 CAS:1266549-31-8 Ossila材料M213

Ossila材料PTB7 CAS:1266549-31-8 Ossila材料M213

產(chǎn)品簡介:Ossila材料PTB7 CAS:1266549-31-8 Ossila材料M213
英國Ossila代理、廠家直接訂貨、原裝正品、交期準時、洽談??!

產(chǎn)品型號:

更新時間:2025-03-31

廠商性質(zhì):代理商

訪問量:2523

服務熱線

0755-23003036

立即咨詢
產(chǎn)品介紹

只用于動物實驗研究等

Applications

PTB7 for high-performance organic photovoltaics.

Poly[[4,8-bis[(2-ethylhexyl)oxy]benzo[1,2-b:4,5-b']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thieno[3,4-b]thiophenediyl]], more commonly known as PTB7.

In stock now for immediate dispatch worldwide.

PTB7 gives some of the highest reported efficiencies for polymer:fullerene solar cells due to its extended absorption into the near infra-red and lower HOMO level. Together with our complete package of processing information, PTB7 becomes a quick and easy way to improve device efficiencies. This represents a cost-effective method to increase performance and impact of devices and data for a wide range of OPV related research.

At typical concentrations for spin-coated devices of 10 mg/ml, a standard batch of 100 mg will produce 10 ml of ink - enough to coat 200 of Ossila's standard sized substrates even assuming 50% ink loss during preparation and filtration. At concentrations of 1 mg/ml (more typical for ink-jet printing and spray coating) up to 100 ml of ink can be produced.

In a standardised reference architecture (using a PEDOT:PSS hole interface and Ca/Al electron interface) we have shown this batch to give a PCE of 6.8% (see data sheet below) and up to 7.4% using PFN. By using new interface materials and architectures PTB7 has been shown to reach efficiencies of 9.2% PCE in the literature [1,2].

The high solubility in a wide range of solvents makes ink preparation and filtration simple, and PTB7 is one of the easiest materials we have ever worked with (simply shake it to dissolve). This also makes it an excellent candidate for a variety of coating techniques including ink-jet printing, spray coating and blade coating.

For information on processing please see our specific fabrication details for PTB7, general fabrication video,general fabrication guide, optical modelling paper on our standard architecture [3], or us for any additional help and support.

References (please note that Ossila has no formal connection to any of the authors or institutions in these references):

  • [1] Enhanced power-conversion efficiency in polymer solar cells using an inverted device structureZhicai He et al., Nature Photonics, V 6, p591–595 (2012).
  • [2] Simultaneous Enhancement of Open-Circuit Voltage, Short-Circuit Current Density, and Fill Factor in Polymer Solar Cells Zhicai He et al., Advanced Materials, V 23, p4636–4643 (2011).
  • [3] Optimising the efficiency of carbazole co-polymer solar-cells by control over the metal cathode electrode Darren C. Watters et al., Organic Electronics, V 13, p1401–1408 (2012)
  • [4] Designing ternary blend bulk heterojunction solar cells with reduced carrier recombination and a fill factor of 77%, N. Gasparini et al, Nat. Energy, 16118 (2016); doi:10.1038/nenergy.2016.118 (Ossila PTB7 was featured in this paper).

Ossila材料PTB7 CAS:1266549-31-8 Ossila材料M213

Datasheet

<:figure style="BOX-SIZING: border-box; TEXT-ALIGN: center; WIDOWS: 1; TEXT-TRANSFORM: none; BACKGROUND-COLOR: rgb(255,255,255); TEXT-INDENT: 0px; MARGIN: 0px; DISPLAY: block; FONT: 14px/20px 'Open Sans', 'Open Sans', 'Liberation Sans', 'Helvetica Neue', Helvetica, sans-serif; WHITE-SPACE: normal; LETTER-SPACING: normal; COLOR: rgb(51,51,51); WORD-SPACING: 0px; -webkit-text-stroke-width: 0px">
 

Chemical structure of PTB7; Chemical formula (C41H53FO4S4)n.

Specifications

Full namePoly[[4,8-bis[(2-ethylhexyl)oxy]benzo[1,2-b:4,5-b']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thieno[3,4-b]thiophenediyl]]
SynonymsPTB7
CAS number1266549-31-8
Absorption670 nm (CH2Cl2), 682 nm (film)
SolubilityChloroform, Chlorobenzene, o-DCB

Ossila材料PTB7 CAS:1266549-31-8 Ossila材料M213

Usage Details

Inverted Reference Devices

Reference device were made on batch M211 to assess the effect of PTB7:PC70BM active layer thickness on OPV efficiency using an inverted architecture with the below structure. These consisted of the below structure and were fabricated under inert atmosphere (glovebox) before encapsulation and measurement under ambient conditions.

Glass / ITO (100 nm) / PFN (6.5 nm) / PTB7:PC70BM (1:1.5) / MoOx (15 nm) / Al (100 nm)

For generic details please see the general fabrication guide and video. For specific details please see the below condensed fabrication report which details the optical modelling and optimisation of the multilayer stack.

Previously it has been shown that PFN of around 6.5 nm gives optimum performance [1-3,P021] while modelling has shown that an Al back cathode gives higher performance than Ag when used with MoOx [4].

The PTB7:PC70BM solution was made in chlorobenzene at 25 mg/ml before being diluted with 3% diiodooctane (DIO) to promote the correct morphology.

Active layer thicknesses of 75 nm, 90 nm and 105 nm were chosen corresponding to the lower, middle and upper end of the "thin film" absorption peak of a typical stack as predicted by optical modelling [1]. For each of these thickness a total of four substrates was produced, each with 4 pixels and the data presented below represents a non-subjective (no human intervention) analysis of the best 75% of pixels by PCE (12 pixels for each condition).

An additional two substrates were also prepared with a methanol wash to help remove the DIO as has been reported in the literature to help improve performance[5].

Overall, the maximum efficiency of 7.2% average PCE (7.4% maximum) was found at 75 nm film thickness.

Note 1: Dektak Thickness calibration

We normally calibrate thin films by use of a Dektak surface profiler, however the use of DIO results in an enhanced level of uncertainty in the film as the DIO will take several hours to fully dry under normal conditions and is likely to undergo some slight further shrinkage when placed in vacuum. The DIO can also be removed by baking the substrate on the hotplate at 80°C for about 10 mins which can be useful for doing quick measurements but also drives excess phase separation between the polymer and PCBM making it unsuitable for device work.

Note 2: Effect of epoxy

Due to the very high solubility of the PTB7 it was noted during fabrication that the film changed colour when in contact with the EE1 encapsulation epoxy in liquid form for extended periods indicating that there was some miscibility. Inspection of the active areas underneath the top cathode indicated that the epoxy had not seeped into the active area before curing and device metrics indicate that this did not appear to affect performance. However, we would recommend minimising contact time between the epoxy and PTB7 films before UV curing.

 

Fabrication

Substrates and cleaning

  • Pixelated Cathode substrates (S173)
  • 5 mins sonication in hot Hellmanex III(1 ml in beaker)
  • 2x boiling water dump rinses
  • 5 mins sonication in warm IPA
  • 2x dump rinses
  • 5 mins sonication in hot NaOH
  • Dump rinse in boiling water
  • Dump rinse in water
  • Stored in DI water overnight and until use

PFN Solution

  • Dissolved at 2 mg/ml
  • Acetic acid dissolved 1:9 in methanol to make stock solution
  • 2 μl/ml of acetic added to solution
  • Stirred for 30 mins
  • Filtered through 0.45 μm PVDF filter

PFN Test Films

  • PFN Test film initially spun at 500 rpm and gave 20 nm
  • Second test film spun at 1000 rpm and gave 16 nm
  • Thickness was extrapolated to 6.5 nm at 6000 rpm

Active Layer Solution

  • Fresh stock solutions of PTB7 (Ossila M211) made on at 10 mg/ml in CB and dissolved with stirbar for 1 hour
  • Mixed 1:1.5 with dry Ossila 99% C70 PCBM to make overall concentration of 25 mg/ml and dissolved with stirbar for 1 hour
  • Old stock solution of 1,8 Diiodooctane mixed 1:1 with CB to make measuring out small quantities easier
  • DIO/CB mixture added to solution to give overall DIO amount of 3%

Active Layer Test Films

  • Test film spun at 1000 rpm for 2 mins using unfiltered solution and dried using methanol before Dektak
  • 1000 rpm gave approximay 85 nm

Active layers

  • Devices spun using 30 μl dynamic dispense (20 μl gave only moderate wetting/coverage)
  • Non methanol devices spun for 2 mins
  • Methanol devices spun for 30 seconds, then coated with 50 μl methanol by static dispense then spun at 2000 rpm for 30 seconds.
  • Cathode wiped with CB
  • Vacuum dried in glovebox antichamber for 20 mins

Evaporation

Left in chamber over the weekend and evaporated with the below parameters.

  • 15 nm MoOx at 0.2 ?/s
  • 100 nm Al at 1.5 ?/s
  • Deposition pressure

Encapsulation

  • As standard using Ossila EE1, 30 mins UV in MEGA LV101

Measurements

  • JV sweeps taken with Keithley 237 source-meter
  • Illumination by Newport Oriel 9225-1000 solar simulator with 100 mW/cm2 AM1.5 output
  • NREL certified silicon reference cell used to calibrate
  • Lamp current: 7.8 A
  • Solar output at start of testing: 1.00 suns at 25°C
  • Solar output at end of testing: 1.00 suns at 25°C
  • Air cooled substrates
  • Room temperature at start of testing: 25°C
  • Room temperature at end of testing: 25°C
  • Calibrated aperture mask of size 0.256 mm2

Standard (Non-inverted) Reference Devices

Reference device were made on batch M211 using a standardised architecture for comparative measurements using Ossila standard substrates and materials. These consisted of the below structure and were fabricated under inert atmosphere (glovebox) before encapsulation and measurement under ambient conditions.

Glass / ITO (100 nm) / PEDOT:PSS (30 nm) / PTB7:PC70BM (variable) / Ca (2.5 nm) / Al (100 nm)

For generic details please see the fabrication guide and video. For specific details please see the below condensed fabrication report and also Watters et al. [3] which details the optical modelling and optimisation of the multilayer stack.

For this standard reference architecture an average PCE of 6.6% was achieved for the optimised thickness with a peak efficiency of 6.8%. Note that no other optimisation was performed (blend ratio, DIO concentration, drying conditions etc) and so further small improvements may be obtained by varying these conditions and significant improvements obtained by using alternative interface materials [1,2].

Efficiency for different PTB7 spin speeds - Standard architecture Jsc for different PTB7 spin speeds - Standard architecture Voc for different PTB7 spin speeds - Standard architecture Fill factor for different PTB7 spin speeds - Standard architectureFigure 3: PCE, Jsc, Voc and FF for standard architecture devices at different spin speeds. Data shown is averaged with max and min overlaid with filled circles (please see note of Dektak measurements). As previously reported [1,2,3], films of approximay 90 nm give the highest performance with greater Jsc and only minor loss in fill factor.

 

PTB7 JV curve for standard architecture
Figure 4: The JV curve for the best performing device - standard architecture.

 

Note 1: Dektak Thickness calibration

We normally calibrate thin films by use of a Dektak surface profiler, however the use of DIO results in an enhanced level of uncertainty in the film as the DIO will take several hours to fully dry under normal conditions and is likely to undergo some slight further shrinkage when placed in vacuum. The DIO can also be removed by baking the substrate on the hotplate at 80°C for about 10 mins which can be useful for doing quick measurements but also drives excess phase separation between the polymer and PCBM making it unsuitable for device work.

Note 2: Effect of epoxy

Due to the very high solubility of the PTB7 it was noted during fabrication that the film changed colour when in contact with the EE1 encapsulation epoxy in liquid form for extended periods indicating that there was some miscibility. Inspection of the active areas underneath the top cathode indicated that the epoxy had not seeped into the active area before curing and device metrics indicate that this did not appear to affect performance. However, we would recommend minimising contact time between the epoxy and PTB7 films before UV curing.

 

Fabrication

Substrates and cleaning

  • Pixelated Cathode substrates (S173)
  • 5 mins sonication in hot Hellmanex (1 ml in beaker)
  • 2x boiling water dump rinses
  • 5 mins sonication in warm IPA
  • 2x dump rinses
  • 5 mins sonication in hot NaOH
  • Dump rinse in boiling water
  • Dump rinse in water
  • Stored in DI water overnight and until use

PEDOT:PSS layer preparation

  • Clevios AI 4083
  • Filtered into vial using Whatman 0.45 μm PVDF filter
  • Spun 6000 rpm for 30 seconds (30 nm)
  • Dynamic dispense of 20 μl using pipettor
  • IPA cathode strip wipe and labelled
  • Put straight onto hotplate at 160°C as soon as cathode wiped and labelled
  • Transferred to glovebox when all samples spun.
  • Baked in glovebox at 150°C for 1 hour

Active layer Solution Preparation

  • Fresh stock solutions of PTB7 at 10 mg/ml in CB and shaken to dissolve
  • Mixed 1:1.5 with dry Ossila 99% C70 PCBM to make overall concentration of 25 mg/ml
  • 1,8 Diiodooctane mixed 1:1 with CB to make measuring out small quantities easier
  • DIO/CB mixture added to solution to give overall DIO amount of 3%

Active layer spin casting

  • Devices spun for 2 mins using 25 μl dynamic dispense
  • Cathode wiped with chlorobenzene
  • Left to dry in glovebox for 2 hours but colour indicated they were still slightly wet
  • Dried in vacuum in glovebox antichamber for 10 mins to remove DIO

Evaporation

Left in chamber over the weekend and evaporated with the below parameters.

MaterialCa
Base pressure8.0 E-8 mbar
Dep start pressure1.7 E-7 mbar
Max pressure2.7 E-7 mbar
Thickness2.5 nm
Rate0.2 ?/s
MaterialAl
Base pressure7.0 E-8 mbar
Dep start pressure6.0 E-7 mbar
Max pressure7.0 E-7 mbar
Thickness100 nm
Rate1.0 ?/s

 Encapsulation

  • As standard using Ossila EE1, 30 mins UV in MEGA LV101

Measurements

  • JV sweeps taken with Keithley 237 source-meter
  • Illumination by Newport Oriel 9225-1000 solar simulator with 100 mW/cm2 AM1.5 output
  • NREL certified silicon reference cell used to calibrate
  • Lamp current: 7.8 A
  • Solar output at start of testing: 0.99 suns at 25°C
  • Solar output at end of testing: 1.00 suns at 25°C
  • Air cooled substrates
  • Room temperature at start of testing: 21°C
  • Room temperature at end of testing: 21°C
  • Calibrated aperture mask of size 0.256 mm2

 

To the best of our knowledge the technical information provided here is accurate. However, Ossila assume no liability for the accuracy of this information. The values provided here are typical at the time of manufacture and may vary over time and from batch to batch.

 


 

在線留言

留言框

  • 產(chǎn)品:

  • 您的單位:

  • 您的姓名:

  • 聯(lián)系電話:

  • 常用郵箱:

  • 省份:

  • 詳細地址:

  • 補充說明:

  • 驗證碼:

    請輸入計算結(jié)果(填寫阿拉伯數(shù)字),如:三加四=7

服務熱線
18123966210

掃碼加微信

欧美日韩亚洲午夜电影-超碰香蕉97com-国产在线一区二区三区在线视频-久久精品综合网91 | 日本人妻中文字幕精品-国产成人精品在线91-熟妇勾子乱一区二区三区-精品人妻久久久中文字幕免费 亚洲高清自拍 99-丁香六月婷婷基地伊人网-91麻豆精品91久久久久久久-欧美日韩一区二区在线 | 精品国产97久久久久久观看高清-91精品久久久久久9s密挑-中文字幕人成乱码中文-国产亚洲一区二区三区av | 91精品夜夜夜一区二区网站-黄色片子在线观看一区二区三区-91久久夜色精品国产九色-蜜臀av一区二区三区精品 | 久久综合伊人色专区-久久久综合狠狠综合-少妇熟女激情一区二区三区-97国产在线小视频 | 久久亚洲成a人片-久久精品视频50-国产又粗又硬又猛的毛片视频-精品视频免费久久 | 久久这里有精品少妇-91精品综合久久久久久久久久-99久久视频在线观看-欧美人妻中文字幕在线 | 亚洲人妻丝袜女老师中文字幕-国产亚洲精品熟女国产成人-亚洲情 中文字幕-日韩乱码中文字幕在线 | 久久久久久久久97精品中文无吗-精品久久久久久久久久欧美-久久久久久久久亚洲中文-97超碰国产亚洲精品 | 人妻精品久久久久中文字幕77-日韩免费毛片变态另-国产精品 中文字幕在线看-久久热99er在线视频观看 | 99久久99久久精品色-久久精品国产久精国产思思-熟妇人妻丰满久久久久久久-天天日天天色天天射天天干 | 国产高国产高潮久久久久久-欧美日韩一区二区三区妖精-国产人妻精品中文字幕-久久国产精品久久伊人91 | 欧美亚洲日本韩国一区-国产三级av在线免费观看-美女av在线免费观看网站-挤进警花两片粉嫩菊蕾蜜月av | av中文字幕亚洲最新-久久人人妻人人人人妻-欧美日韩亚美一区二区-91精品夜夜夜一区二区快速播放 日韩av在线不卡更新官网-国产av精品麻豆高清在线观看-内射极品美女亚洲一区-日韩人妻中文字幕在线一区 | 97超频视频在线播放-九九久久男人精品视频-精品久久久久久国产-韩国视频在线观看一区二区 | 2021中文字幕在线观看-91成人在线观看潮喷蘑菇-久久久久久久久99精品_国产-婷婷综合久久av | 成人av大片免费看-就是色亚洲精品懂色-欧美精品日韩久久亚洲综合-日韩黄色av一区二区三区 | 久久人妻日韩蜜桃精品-日韩中文字幕美女人妻-日韩av在线播放导航-麻豆精品一区二区三区四区 | 成人日韩电影在线-日韩av在线播放链接-日韩午夜精品在线视频-久久人人妻人人爽人人 | 国产情色av一区二区三区-欧美黑人性猛交xxxx免费看-2023中文字幕在线视频-国产日韩欧美高清精品 欧美精品国产久久久久-亚洲男人的天堂色偷偷-欧美日韩亚洲清纯-中文字幕国产视频91 | 婷婷久久综合中文字幕-久久人妻少妇嫩草av蜜桃动态图-人妻少妇精品中文字幕视频-国产精品麻豆成人av网 | 日韩97久久久-久久精品国产亚洲-久久99精品国产.久久久久-日日躁18摸日日摸夜夜爽 | 国模精品一区二区三区视频-亚洲精品人妻插插插-久久久久看中国免费观看视频-久久婷婷人人澡人人爽人人喊 | 91啪啪啪在线视频-国产精品久久久久粉嫩小久久-乱中年女人伦av一区二区-在线视频中文字幕激情 | 中国精品一区二区三区四区视频-久久久久久国产精品频道-久久精品15久久久-中文字幕一区三区人妻 国产欧美日韩在线激情-亚洲一区在线观看免费观看-精品熟女一区二区在线-丁香花开五月激情久久视频 | 99国产精品性色内射-久久久人妻精品一区二区三区四区-欧美国产成人久久精品直播-亚洲国产精品wwww | av一区二区三区东京热-丰满白嫩人妻一区二区三区-亚洲欧美色中文-老熟女五十路乱子交尾中出一区 日韩中文字幕av色电影-婷婷综合婷婷综合-日韩av在线播放第一页-乱色熟女一区二区三区1000部 | 日韩欧美国产精品免费-国产在线手机版在线-久久精品国产99精品国产-99精品热在线在线观看视频 | 91性高湖久久久久久久久久久-另类亚洲欧美视频日本-伊人久久大香线蕉综合色狠狠-亚洲精品乱码久久久久久按摩1 | 三级黄色片av在线观看-中文字幕乱偷人妻一二三区蜜臀-麻豆国产一区二区三区四区-久久精品国产色蜜蜜麻豆国语版 | 日韩欧美中文字幕丝袜-久久99国产精品99久久-久久久久久久久久久久久欧美-亚洲欧洲日产国码av天堂偷窥 | 国产伦精一品二品三品视频网址-99精产国品一二三区别-亚洲伊人久久久久久久-人妻精品一区二区免费 | 亚洲欧洲成人久久桃色一区二区-91亚洲精品台湾佬-久久久在线播放-美女激情久久久 | 国产精品久久久尤物-日韩精品人妻免费看-婷婷久久 不卡-一区二区三区中文字幕高清 | 国产精品久久久久久久久久福利-大吊视频一区二区三区四区-2022国产成人精品视频人-亚洲欧美日韩成人免费 | 99久久久久久久久-久久玩人人妻潮喷-人妻精品一区二区蜜桃-99久高清在线观看视频一 | 欧美一区二区熟妇-久久久国产成人一区二区三区-亚洲av官网久久-在线观看亚洲麻豆 | 婷婷综合五月在线-日本中文字幕在线网-丝袜亚洲一区在线-日韩毛片在线视频观看 | 日韩中文在线免费视频-日韩在线有码中文-91久久久久一区二区-黑人巨大精品在线观看 | 欧美激情一区二区三区一在线-欧美黑人巨大精品高清视频在线观看-在线视频中文字幕成人欧美-久久天天躁夜夜躁狠狠85麻豆 | 久久99精品久久久久久人妻-久久久亚洲视频区-91精品一久久香蕉国产线看-久久这里有精品999 |